Finishing
Type III hard anodising is the finish that lets an aluminium part do a steel part’s job. It is also the finish most often specified without allowing for what it does to the dimensions — and that is where the arguments start.
Quick answer
Hard anodising grows a ceramic oxide into the surface, typically 25–50 µm thick. About half grows inward and half outward, so a bore shrinks and an outside face grows. Mask threads, bores and sealing faces, put the growth allowance on the drawing, and approve a coated first article before the batch. Type III is for wear and corrosion, not for a colour match.

What Type III actually is
Anodising is an electrochemical process that converts the aluminium surface into an oxide layer. Type II is the decorative version: a thinner coating, usually 5–20 µm, with a porous structure that accepts dye. Type III, often called hardcoat or hard anodising, uses a colder bath and a higher current to grow a denser, thicker layer, typically 25–50 µm. It is much harder and more wear-resistant, and it is usually dark grey to black rather than a bright colour.
The layer is not paint. It is part of the metal: it grows from the substrate, bonds to it, and cannot peel like a coating. That is why it resists wear and corrosion so well. It is also why it changes the dimensions: the oxide occupies more volume than the aluminium it replaces, so the surface moves outward and the substrate moves inward.
The practical rule is roughly 50/50. A 40 µm coating adds about 20 µm to an outside face and removes about 20 µm from a bore, per surface. The exact split depends on the alloy, the bath and the coating thickness, which is why a coupon matters more than a table.
What it does to your dimensions
| Feature | What changes | What to do |
|---|---|---|
| Outside face | Grows by roughly half the coating thickness | Allow the growth on the drawing, or finish-machine after masking |
| Bore | Shrinks by roughly half the coating thickness per side | Mask the bore or specify the fit after coating |
| Thread | Coating builds on the flanks and crests | Mask threads or use an oversized thread allowance |
| Sealing face | Surface becomes hard and slightly rough | Mask, or specify a finish and flatness after coating |
| Sharp edge | Coating builds and can crack or chip | Break edges; specify a radius |
| Deep blind hole | Throwing power is limited; coating may be thin at depth | Tell the finisher the depth; consider masking |
A 20 mm H7 bore is the classic example. The hole is machined to the top of the tolerance, the coating grows inward, and the bearing will not fit. The fix is not to “machine it bigger” by guesswork; it is to mask the bore or to specify the fit after coating and let the finisher prove it on the first article.
Outside dimensions have the opposite problem. A part that must fit inside a housing can grow by 20–25 µm per face, which is enough to turn a sliding fit into an interference fit. If the outside is cosmetic and the fit is inside, mask the fit and coat the visible face.
What the coating does to a bore and an outside face
The diagram is the reason a hard-anodised bore needs a masking note. The oxide does not sit on top of the surface; it grows from it. A 40 µm coating moves the outside face out by about 20 µm and the bore in by about 20 µm per side. If the drawing does not say which surfaces are masked, the finisher will choose, and the bearing may not fit.
Which aluminium alloys behave
6061-T6 is the default. It anodises predictably, takes a uniform dark grey, and is available in plate, bar and extrusion. Most hard-anodised machined parts we see are 6061.
7075-T6 hard-anodises, but the colour is darker and less uniform because of its copper and zinc content. It is a good choice when strength matters, but if the part is cosmetic, approve a coupon. The coating can also be more brittle on thin sections.
2024 contains copper and has lower corrosion resistance; it can be hard-anodised, but the substrate is less forgiving in a wet environment. If the part is structural and exposed, consider a coating system or a different alloy.
5083 is a marine alloy with good corrosion resistance; it anodises, but the colour and hardness differ from 6061. Do not assume a colour match across alloys.
Castings are the hardest case. Porosity, silicon content and surface condition can produce a patchy coating. If the part is a casting, tell the finisher and approve a coupon before the batch.
Design rules for hard anodising
- Break sharp edges. A hard coating on a knife edge is fragile; a 0.3–0.5 mm radius helps the coating build evenly.
- Mask threads and bores. A masked thread is cheaper than a thread that will not start. If the thread must be coated, specify an oversized allowance and prove it on the first article.
- Do not rely on the coating for electrical conductivity. Hard anodising is an insulator. If the part needs a ground path, mask the contact area or add a masking note.
- Think about throwing power. Deep blind holes and narrow slots may not coat fully. Tell the finisher the depth and the minimum coating at the bottom.
- Do not use Type III for a colour match. It is a dark grey/black functional coating. If the customer wants a colour, Type II or powder coating is the right conversation.
- Allow for the growth in the fit. The drawing should say whether the fit is before or after coating, and which surfaces are masked.
How we specify and inspect it
We machine the part and manage the anodising through a finishing partner we have used for years. The quote includes the masking plan and the growth allowance; it is not an afterthought. For a first order we send a coupon in the production alloy and the production finish, and we check the coated first article before the batch is released.
On the shop floor, the checks are simple and practical. A blade test on a corner tells you whether the coating is Type II or Type III; a coating-thickness gauge gives a number; a bore gauge or pin confirms the masked fit. If the coating is on a sealing face, we check flatness after coating, not before.
We are not a finisher and we do not pretend to be. What we control is the drawing, the masking plan, the first article and the inspection. That is the part that decides whether the coated batch fits.

When Type III is the wrong answer
The part is cosmetic. Hardcoat is dark and functional. If the customer wants a bright colour, use Type II or powder coating.
The fit is tight and cannot be masked. A 20 µm growth per surface can close a bearing fit. If the bore cannot be masked, the part may need a post-coat hone or a different finish.
The part needs electrical conductivity. Hard anodising insulates. Mask the contact areas or use a conversion coating instead.
The wall is very thin. The coating is ceramic and can crack under impact or bending. A thin wall may need a different alloy or a different finish.
The part is a casting with porosity. The coating may be patchy. A coupon and a sample batch are the only honest way to know.
Pain points we see on hard-anodised parts
The bore was machined to nominal. After coating, the bearing will not fit. The drawing did not say the bore was masked or that the fit was after coating.
The thread was not masked. The first thread starts hard, the second galls, and the customer blames the tap. The coating built on the flanks.
The colour does not match the last batch. Hardcoat is not a colour process. If the customer expects a match, the specification is wrong.
The edge chipped. A sharp corner concentrates the coating and cracks. A small radius would have prevented it.
The coating is thin at the bottom of a blind hole. Throwing power is finite. The drawing asked for 50 µm everywhere without saying how deep the hole was.
What thickness should I specify?
The right thickness is the one that survives the wear or corrosion duty without closing the fit. Use the table as a starting point, then prove the fit on a coated first article.
| Coating thickness | Typical use | Dimensional effect |
|---|---|---|
| 25 µm | General wear, light corrosion | About 12 µm per surface |
| 40 µm | Sliding wear, outdoor parts | About 20 µm per surface |
| 50 µm | Heavy wear, abrasive contact | About 25 µm per surface |
| 80 µm | Severe wear, salvage of a worn part | About 40 µm per surface; masking is essential |
The drawing should state the thickness range, the alloy, the masking and the fit condition. “Hard anodise” alone does not tell the finisher what to grow or what to protect.
How do I mask threads and bores?
Masking is a drawing decision. Mark the threads, bearing bores, sealing faces and grounding points that must stay bare. The finisher will plug or tape them; the machinist will leave the allowance if the feature is coated.
For a thread, the choice is mask it, use an oversized allowance, or re-tap after coating. Masking is the most reliable for small threads; an allowance is common for larger threads. For a bore, mask it or specify the fit after coating. A 20 µm growth per side is enough to turn a sliding fit into an interference fit.
If the part has a masked face and a coated face on the same side, say which is which. A photo with a marker is often clearer than a note.
What drives the price of hard anodising?
| Driver | Why it matters |
|---|---|
| Surface area | More area, more current and time |
| Thickness | Thicker coating runs longer and is more sensitive |
| Masking | Threads, bores and faces add labour |
| Alloy | Some alloys are harder to coat uniformly |
| Batch size | Rack minimum and colour/line changes |
| Cosmetic requirement | Handling, rack marks and colour uniformity |
On a small batch, the rack minimum and the masking can dominate. Ask for the finishing line separately from the machining.
A real example: a 6061 housing with a 30 µm bearing bore
An instrument housing in 6061-T6 had a Ø30 H7 bearing bore and a cosmetic outer face. The drawing said “hard anodise, black” with no thickness or masking. The first batch came back with the bore 0.04 mm tight; the bearing would not fit.
We changed the drawing to 30–40 µm, masked the bore, and specified the outer face as cosmetic. The next batch was coated and the bore was checked with a pin gauge after coating. The bearing fitted, and the outer face passed the colour sample.
The lesson: the coating thickness and the masking are part of the drawing, not a note for the finisher. A 30 µm coating is not a number you can add after the part is machined.
Before you send a part for hard anodising
- Alloy and temper.
- Thickness range and cosmetic/functional requirement.
- Masking drawing for threads, bores and sealing faces.
- Fit condition: before or after coating.
- Colour and surface finish, with a coupon if cosmetic.
- Batch size and finishing minimum.
FAQ
How thick is Type III hard anodising?
Typically 25–50 µm, with heavier coatings up to 80 µm for severe wear. The exact thickness should be specified on the drawing and proved on a coupon.
Does hard anodising change the dimensions?
Yes. About half the coating grows inward and half outward. A bore shrinks and an outside face grows by roughly half the coating thickness per surface.
Can I anodise a thread?
You can, but the coating builds on the flanks and can make the thread tight. Most production parts mask threads or use an oversized allowance.
Is Type III the same as black anodising?
No. Type III is a functional hardcoat, usually dark grey/black. Black Type II is a decorative dye. They have different thickness, hardness and dimensional effects.
Can you anodise 7075?
Yes, but the colour is darker and less uniform than 6061. If the part is cosmetic, approve a coupon first.
Do you anodise in-house?
No. We machine in-house and manage anodising through a long-term finishing partner. The masking plan, coupon and first-article check are ours.